TIG
Advice 1
We all talk about current flowing through circuits from the positivve terminal to the negative terminal – but there is no such thing as a current.
Electricity is the flow of electrons, tiny negative charges which flow from negative to positive.
For this reason I use the term 'electron-flow' where others use 'current'.
Advice 2
This chapter is an edited version of that found on Welding.org. If you can access that website, please do. It has many more articles, and those are illustrated with colored photographs. This site is for underprivileged students with poor internet connections which require brief download times. Thus they are unable to use welding.org because its articles are too large (3.4MB to this 40KB). You are slowing their downloads, risking a dropped connection. If you re-address, then thank you.
What is TIG Welding ?
TIG Welding is a manual welding process that requires the welder to use two hands to weld. What separates TIG welding from most other welding processes is the way the arc is created and how the filler metal is added! When TIG Welding one hand is used for holding the TIG torch that produces the arc and the other hand is to add the filler metal to the weld joint. Because two hands are required to weld; TIG welding is the most difficult of the processes to learn, but at the same time is the most versatile when it comes to different metals. This process is slow but when done correctly produces the highest quality weld. TIG welding is used mostly for:
- critical weld joints
- welding metals other than common steel
- where precise small welds are needed.
TIG Welding Names
Knowing alternative names and abbreviations for TIG welding is important for anyone who is interested in getting a job as a TIG welder. Many companies may use alternative names when placing ads in the classifieds. Sometimes they may use alternative name on a written test to test your knowledge of the welding process. Besides that the alternative name means something to the process. As of today TIG welding is the slang term that is widely accepted and used. TIG stands for Tungsten Inert Gas Welding.
TIG welding's proper name is Gas Tungsten Arc Welding or "GTAW". This is the name the American Welding Society and other welding organizations refer to this process on their welding procedures. GTAW is also the abbreviation that welding engineers use to specify the welding process that is to be used on blue prints. On top of that; when working on high pressure piping you could get sent home for a few days for not using proper terminology!
Why Use Tungsten to Weld ?
Tungsten:
- Physical: very hard, slightly radioactive, and brittle metal. Can break a tungsten electrode with just a tap of a hammer.
- High MPt, high conductivity: gives an arc up to 6,000oC (11,000oF), hotter than its own melting point
- Tensile strength: up to 500,000psi (commonly used steel has 36,000psi of tensile strength)
- Uses: non-consumable TIG electrodes, light bulbs, heating elements, rocket engines; any place that requires a very high melting point or the need to pass electricity at a high temperatures.
How TIG Welding Works
TIG welding requires three thing:
- heat
The heat is produced by electricity passing through the tungsten electrode by creating an arc to the metal.
- shielding
The shielding comes from a compressed bottle of gas that flows to the weld area to protect it from air.
- filler metal
The filler metal is just a wire that is dipped by hand into the arc and melted.
The method:
- The welder turns on the gas flow, by a valve on the TIG torch itself. The gas begins to flow and starts protecting the weld area from the air.
- The torch is held over the weld joint just far enough for the torch not to touch the metal.
- The welder presses a foot pedal and the TIG torches tungsten electrode starts an arc.
- Once the arc is started the two pieces of metal begin to melt by creating a puddle of metal.
- Once the puddle is established the welder with the other hand starts filling the joint by manually dipping a welding wire into the arc to fill the joint.
Finally this process creates a single piece of metal.
TIG Power Supplies
TIG Power Supplies:
- Dynasty 350 TIG Power Supply
TIG welding power supplies are usually Stick welding power supplies, with a few extras added on. A stick welding machine needs only a basic TIG torch to weld well (with a bottle of argon, of course). Both welding machines are constant amperage power supplies, keeping the amperage consistent and the heat settings regulated in amperage. The voltage on these power supplies will vary depending on the length of the arc.
TIG power supplies often come with a feature called a “high frequency start”. This eliminates the need to physical strike an arc. Once the TIG torch is activated the high frequency start feature will can literally create an arc across a one inch gap between the TIG torch and the metal! This is done by creating a brief moment of high voltage that has the pressure required to jump the distance. Once the arc is established the voltage drops and the amperage goes to what the machine is set at. Thiskeeps the tungsten free of contamination and used up. The high frequency start feature helps the tungsten electrode live up to its designation as a non-consumable electrode.
- Syncrowave 300 TIG Power Supply
Some common feature for TIG welding power supplies are:
- perflow: gives the shielding gas a pre flow time to shield the weld area before the arc is started
- postflow: keeps the gas flowing for a set time after the arc is stopped to keep the weld are protected until the weld cools.
Other features of TIG welding power supplies are frequency settings that help the characteristics of the welding arc. There are many ways to help the welding arc run smoother. Some of the features do this by using frequency ranges and/or pulses of electricity to achieve the desired arc type. The biggest benefits of these features are they give the arc a cleansing action. These settings are not commonly used unless welding aluminium or magnesium.
Voltage types and polarities
TIG welding uses the same voltage types as stick welding. The two voltage types are:
- DC Direct Current like the current from a car battery that only flows in one direction. That is from the (-) negative side to the (+) positive side.
- AC Alternating Current like the current in your home. This current goes back and forth. To go back and forth once, is one cycle; your domestic supply is probably about 50 cycles per second (Hertz).
TIG DC welding uses two polarity types.
The polarity determines whether most heat goes to the metal or to the electrode.:
- DC Direct Current Electrode (-) Negative (DCEN). This means the electrode or welding handle is the negative side of the circuit and the electrons flow from torch to metal. The heat follows the direction of the electrons.
DCEN (-) electrons flow electrode => metal . . . heats metal
DC electrode (-) negative concentrates about 2/3s of the heat onto the metal welded. This produces a deep penetration weld.
- DC Direct Current Electrode (+) Positive (DCEP). This means that the electrode or welding handle is the positive side of the circuit and the electrons flow from the metal to the TIG torch.
DCEP (+) electrons flow metal => electrode . . . heats electrode
DC electrode (+) positive concentrates about 2/3s of the heat onto the electrode. This produces a shallow weld that is more suitable for sheet metal and at the same time gives the arc a cleansing action.
Convert a Stick Welder into a TIG Welder
It is very common in the field to use a Stick welder to TIG weld pipe. This is what most big companies use to TIG weld carbon and stainless steel pipe. I think Stick welding power supplies do a better job then TIG welding power supplies when it comes to heavy wall pipe.
The actual conversion is very easy and only requires an air cooled TIG torch and a bottle of Argon.
For most welding applications there will be three steps involved to start TIG welding:
- change the polarity to DCEN(-)
- take an air cooled TIG torch and hook it up to the stinger or electrode holder
- take the gas supply hose and attach it to the regulator on a bottle of Argon.
That's all !
Torch types
When it comes to TIG welding there are two options for choosing a torch:
- an air cooled torch which is the least expensive and most practical. The down side to the air cooled TIG torch is it heats up and much of the heat the arc produces is wasted. After ten minutes the handle becomes too hot to hold.
- a water cooled torch is more efficient but requires a water cooler and additional maintenance.
Remote Start vs. Manual Start
Once a TIG torch is chosen there are two options on how to start the arc:
- manual start
First there is the simple way of manually starting the arc. Just like a Stick welding once the TIG welding machine is turned on, so is TIG torch. The arc is started by manually striking the metal with the tungsten.
- remote start
The second option is remote start. Remote start features come in two different forms:
- a switch on the torch: Hand operated remote starts are very simple; just a button taped onto the torch and pressed with a finger to operate the remote start cable connected to the welding power supply. That activates the high frequency start feature, makingstarting the arc easier and keeping the tungsten from being contaminated.
- foot pedal operated: Foot operated or foot pedal remote starts are more complicated. They control both the high frequency start and the amperage. They suit shop work where the welder can sit. It is very difficult to weld standing with a foot pedal remote start. The upside to a foot pedal remote start is you have full control over the heat with which you are welding.
Shielding gases
Gases protect the weld area from air contaminating the weld. The two most commonly used gases to TIG weld are:
- Argon / Ar (typically used)
- Helium / He
Since Argon and Helium are Noble Inert Gases they do not change the characteristics of the weld joint. In some rare cases there are three types of mixture used:
- argon and hydrogen
- argon and nitrogen
- argon and helium (for deeper penetration on thicker plates).
However, pure Argon will cover almost all welding needs.
Tungsten Electrode Types
As the name states “Tungsten Inert Gas Welding” tungsten is the main ingredient in the electrode. What changes is there are very small percentages of other metals added to help create the desired arc characteristics. The common metals added to Tungsten are Cerium, Lanthanum, and Zirconium. The following Tungsten mixtures are the most widely used:
- Pure Tungsten, EWP
Pure Tungsten is used with AC alternating current for welding aluminium and magnesium only. It comes with a green colored tip with an AWS (American Welding Society) classification code of “EWP” on the package.
- 0.25 % to 0.5% Zirconium Tungsten, EWLa-1
Zirconium Tungsten has similar properties to pure Tungsten. Zirconium Tungsten comes in a mixture form ranging 0.25%–0.5% Zirconium Oxide and the rest is Tungsten. It is typically used with AC alternating current for welding of aluminium and magnesium. It comes with a brown colored tip and an AWS classification of EWLa-1 on the package.
- 1% Thorium Tungsten, EWPTh-1
Thoriated Tungsten is typically DCEN. The added Thorium Oxide helps the electrode carry more current at a lower temperature while making arc starting a bit easier. Thoriated Tungsten is used for welding most metals besides aluminium and magnesium. Some of the metals it works well on are carbon steel, stainless steel, chromium alloys, nickel, and most other ferrous metals. The percentages of Thorium Oxide added typically range from 1% to 2%. 1% Thoriated Tungsten comes with a yellow colored tip and has an AWS classification of EWTh-1 on the package.
- 2% Thorium Tungsten, EWPTh-2
2% Thoriated Tungsten comes with a red colored tip and has an AWS classification of EWTh-2 on the package.
Electrode Diameters
With TIG welding the electrode size is not the most critical component of the process, as long as it is used only within its amperage rating. What matters the most is the shape of the tip and that determines the arc characteristics. For most uses any size between 1/16 to 1/8 of an inch electrode diameter will do. The more common sizes on the market are:
- 1.5mm (1/16")
- 2.25mm (3/32")
- 3mm (1/8")
- 3.75mm (5/32")
- 4.5mm (3/16")
- 6mm (1/4")
Shaping Electrodes
Since Tungsten comes in a rod form with a square cut end it needs to be shaped. Some of the tip shapes used in these electrodes are:
- Pointed Tungsten Electrodes
A pointed tip is typically used in welding ferrous metals like steel. The current used is DCEN (direct current electrode negative). This allows the current to flow from the electrode to the metal, which concentrates the arc temperature onto the metal. The pointed tip in this case will keep its shape by maintaining a higher arc temperature than the electrodes melting point. If the polarity were reversed the tungsten would likely start melting.
Shaping of a pointed electrode is typically done on a grinding wheel or Tungsten electrode sharpener. When using a grinding wheel it is best to use a fine grit wheel that is only to be used for sharpening Tungsten electrodes. Since Tungsten is slightly radioactive do not inhale the particles.
To sharpen the electrode, point it upward while slowly and lightly rolling it on the grinding wheel between your fingers to obtain a round point. Do not wear gloves lest the glove be pulled into the grinding wheel.
A Tungsten electrode sharpener it is much like a pencil sharpener, and much easier and safer.
- Rounded and tapered-ball-end Tungsten electrodes
Rounded or tapered-ball-end electrodes are typically used for welding non-ferrous metals like aluminium and magnesium. The current used to weld these metals is AC (alternating current). The rounded or tapered-ball-ended electrode helps by spreading the arc over a wider area of the electrode. To get a round or ball shaped end to an electrode:
- use DCEP (direct current electrode positive)
- turn on the Argon gas and if possible start an arc on a piece of copper; or use very clean metal
- the tungsten will begin to melt once the amperage is high enough and then start to create a droplet at the end of the electrode
- Once you get the proper size ball at the end of the electrode, stop the arc
- after the shape is obtained turn the power supply back to AC.
In some other cases a rounded or tapered-with-a-ball-end electrodes can be used for welding sheet metals with DCEP (direct current electrode positive). What this does is concentrate 2/3s of the heat on the tungsten electrode and prevent blowing holes in the sheet metal. When using DCEP avoid too much current which burns up the tungsten.
TIG Cup Sizes
Cup sizes come with a standard coding system.
The coding system uses #1 = 1/16" = 1.5mm.
For example a # 5 cup is 5/16" or a #9 cup is 9/16". The number used on the cup is the number of 16ths of an inch. The metric version, as always, will be easier. (300 million people have lost so much learning time in school by being compelled to master the US imperial system of meazurement. With this attitude of its leaders that the US leads and the rest of the world must follow, it is little wonder that the US empire is already in decline; and they cannot even see it.)
Filler Wire Designation
Just like any other welding process the filler wire for TIG welding has a designation coding system. Since TIG welding does not use any flux, the designations are pretty simple. In most cases you can use MIG welding wire. The only difference between MIG welding wire and TIG welding wire is the way they are packaged. Typically TIG welding wire comes in 36” lengths. A common welding wire for mild steel is ER70S-2.
The designation code is as follows:
- ER - An electrode or filler rod that is used in either a wire feed or TIG welding.
- 70 - A minimum of 70,000 pounds of tensile strength per square inch of weld.
- S - Solid wire.
- 2 - The amount of deoxidizing agent and cleansing agent on the electrode.
TIG welding wires come in many sizes and these are the more common diameters:
- 1.5mm (1/16")
- 2.25mm (3/32")
- 3mm (1/8")
- 3.75mm (5/32")
- 4.5mm (3/16")
Joint Set-Up
Joint set-up is extremely critical when it comes to TIG welding. There cannot be any rust, oxidation, mill scale, paint, oil, or anything that does not belong there except for the bare metal. All joints must be cleaned with a grinder or in the case of some metals like aluminium, a chemical cleaner is used. In some factories every piece to be welded gets an acid bath. TIG welding arguably produces the best weld quality but that weld quality depends upon a clean joint.
Purging
Purging is a common term when it comes to TIG welding pipe. What purging does is replace the air in a pipe with a gas that will not react with the root of the weld.
Purging prevents weld oxidation or in pipe welder slang “sugar". When interviewing for pipe TIG welding jobs a common question asked is “How do you prevent sugar”? In other cases when welding, a box can be filled with Argon to weld in it. Argon is heavier then air so it will fill a box or shape just like water.
Argon can also be dangerous when the proper ventilation is not used. If you are in a sealed room and you have a bottle of Argon leaking, it will fill the room from bottom up, just like water would. You cannot see or smell it. Once the Argon fills the room you will be breathing and suffocating at the same time, while not even knowing it! Typically Argon is used to TIG weld but since it is very expensive it is not used by itself to purge pipe. What most people use to purge a pipe is Nitrogen or CO2 gas.
Pipe Purging
Purging is to remove all oxygen.
Purging pipe typically requires the use of math. In some cases like in shipyards they have charts that say what pipe size, length, CFH (cubic feet an hour of gas flow) is needed, and the time required to purge the pipe.
How to Purge Pipe
How to Purge Pipe:
- Before purging the pipe the open area of the pipe needs to be sealed off. That also includes the weld area. This is done by taping to area and when it is welded the tape is pulled away in small sections.
- Once the area is sealed off put a vent hole at one end of the pipe opposite the tube filling the pipe. The location of the vent hole will vary depending on if you are using Helium or Argon:
- Argon is heavier than the air. Vent at the top of the pipe.
- Helium is lighter than the air. Vent at the bottom of the pipe.
The best way to meazure a pipe:
- take the inside diameter and halve it to get the radius.
Radius = diameter/2
- Cross-sectional area = π x radius x radius = 3.14 x ? x ?
- take the length of the pipe
- Volume = length x cross-sectional area
Some gas-flow instruments will meazure in cubic feet (so you meazure the pipe in inches) and some in cubic metres or cubic centimetres (so you meazure in mm).
Dimensions:
- mm: to convert mm3 to cm3 divide by 1000
- mm: to convert mm3 to m3 divide by 1000 and by another 1000 and by another 1000. Small isn't it ?
- inches: to convert to cubic feet, divide by 1728 (= 12" x 12" x 12")
If your gas flow instrument meazures in CFH (cubic feet per hour) all you have to do is time the flow rate to the cubic feet of filler gas needed.
TIG Welding Machine Set-Up
When setting up a TIG welder there are two main settings:
- amperage
Amperage settings vary depending on the type and thickness of the metal to be welded.
- gas flow
Gas flow rates also vary depending on draft conditions, cup size, and sometimes the position of the weld. The gas flow rate could range from 5 CFH to 60 CFH for a large cup and drafty conditions.
When choosing the gas to weld it is almost always assumed that you will be using pure Argon.
Some basic guidlines for machine set-up are as follows:
- 1.5mm (1/16") Tungsten - Require an amperage rage between 50 to 100 amps. The recomendated cup sizes are 4, 5, or 6. Gas flow rate should be between 5 to 15 CFH.
- 2.25mm (3/32") Tungsten - Require an amperage rage between 80 to 130 amps. The recomendated cup sizes are 6, 7, or 8. Gas flow rate should be between 8 to 20 CFH.
- 3mm (1/8") Tungsten - Require an amperage rage between 90 to 250 amps. The recommended cup sizes are 6, 7, or 8. Gas flow rate should be between 8 to 25 CFH.
Welding steel
Tig welding steel is very easy. The polarity typically used is DCEN (direct current electrode negative), Argon gas, and Thorium Tungsten. For welding steel and stainless steel the Tungsten needs to be shaped to a fine point.
Welding stainless steel
Stainless steel welds almost like steel. It does not take a lot of extra practice, anduses the same type of tungsten with Argon gas.
The one exception is that welding stainless steel requires good gas coverage. Stainless steel sometimes requires the weld to be submerged in an Argon bath or if it is an open root weld the inside of the joint must be purged with a filler gas.
Stainless steel has a tendency to warp with too much heat or insufficient bracing. Control by staggering the welds and bracing the weld area frequently.
A good stainless steel TIG weld will have a copper color. A gray or dark color weld comes from being too slow or too hot.
Sanding disk for cleaning stainless steel
When TIG welding stainless steel, joint preparation is extremely important. The joint must be absolutely free of anything except clean stainless steel. If this is not done you will find the filler wire will not flow into the joint. When welding on a less than clean stainless steel joint the filler wire will not stick to many parts of the joint. To avoid this it is best to hit the joint with a sanding disk or a file.
This is true on multi pass welds too. If you put in one bead and then need to put in a second pass you also need to clean that area again before welding.
Welding aluminium
When TIG Welding aluminium:
- The tungsten needs to be either pure Tungsten or Zirconium Tungsten.
- The tungsten also needs a ball shape at the end of it to spread the heat properly.
- aluminium always welds with AC (alternating current). Welding aluminium always requires a high frequency start from either a high production button or a foot pedal operated TIG torch.
- The main difference when welding aluminium verses other metals is how the puddle looks. aluminium just has a shiny puddle that does not glow. It looks like tinfoil moving.
- Avoid overheating the aluminium; or the whole weld area will just drop to the floor.
Welding anodized aluminium
When TIG welding smaller diameter aluminium tubing, many people like to use a high production button. The purpose for the button is to bump the weld, which is basically spot welding around the pipe or tubing.
This technique is typically used to weld anodized aluminium pipe. In the yacht industry many boats have tuna or marlin towers installed before they are sold. These towers are made of brushed or anodized aluminium to keep the pipe protected from the salt water. The anodized pipe has a coating that makes it very difficult to weld.
Welding anodized aluminium requires two steps:
- spot weld around the pipe and add filler wire. This weld is less than acceptable looking because the anodized coating has not melted properly.
- spot or bump weld around the same weld without adding filler wire. What this does is melt the anodized coating into the weld better.
- paint with weld paint to protect it.
Welding exotic metals and alloys
TIG can weld almost any metal. This is possible because the main Gases used are noble inert Gases and their properties do not alter the weld properties. Most other welding processes use some type of flux or chemical additives to the filler metal. With TIG welding it is pure heat that creates the weld joint and that allows any metal that can be melted to be joined as long as the filler wire is compatible. Some of the exotic metals that are commonly welded are::
- Copper Nickel “CUNI” and Copper Nickel Alloys
TIG welding copper and copper nickel alloys are typically done with pure Argon and sometimes Argon / Helium (75% Ar /25% He) gas mixture. In most cases the tungsten type used will be 2% Cerium with an orange color and an AWS classification of EWCe-2. In other cases 2% Thorium tungsten can be used. The most common welding current and polarity is DCEN (direct current electrode negative).
Many people who weld CUNI say it has a muddy feel to it. That is only true if you use too much heat and in that case the metal will turn very dark. When done right the weld will look very close to stainless steel with almost the same copper color to it. The best way to describe the feel and look of the puddle is a combination between stainless steel and aluminium. The puddle acts like stainless steel but is more fluid with a hint of shine or tin feel like welding aluminium.
The catch with welding copper nickel and copper nickel alloys is that cold lap and roll are a common problem. Many time the weld looks like it has penetrated properly but in some places it is actually lacking penetration. It is very hard to detect cold roll and lap with copper nickel unless a die penetration test is done.
When it comes to open root welds on copper nickel there is a different technique used. You need to keyhole the root open on the joint! Not a joke! You strike your arc and then create a keyhole followed by dipping the filler wire into it. You just keep repeating this till the root is finished. It may sound difficult but the filler wire puts in a very smooth root with good penetration on the backside.
- Magnesium
Magnesium is typically welded with pure Argon gas. The type of tungsten used is typically Zirconiated tungsten with an AWS designation of EWZr. In most cases the current will be AC (alternating current) requiring a high frequency start.Magnesium is typically welded with pure Argon gas. The type of tungsten used is typically Zirconiated tungsten with an AWS designation of EWZr. In most cases the current will be AC (alternating current) requiring a high frequency start.
- Titanium
Welding titanium uses Argon gas and many times requires an Argon bath to be welded in. In many cases the gas coverage gives is not enough. Titanium can be welded using 2% Thorium Tungsten with an AWS classification of EWPTh-2 and with DCEN (direct current electrode negative).
Dissimilar metals
TIG welding has a lot of options when it comes to welding dissimilar metals, mostly depending on the design of the filler wire. In a few cases there are two steps to welding dissimilar metals but in the end these metals can be joined. Some of the combinations of dissimilar metals that can be TIG welded are:
- Copper to Everdur
- Copper Nickel to EverdurCopper Nickel to Everdur
- Copper and Everdur to Steel
- Copper to Stainless Steel
- Hastelloy Alloy C to Steel
- Nickel to Steel
- Stainless Steel to Cast Iron
- Stainless Steel to Inconel
- Stainless Steel to Low Alloy or Carbon Steel
Welding techniques
Many of the standard patterns apply to TIG welding techniques. What really changes is the way the filler rod is added and the fact that you need to use both hands at the same time. The filler rod should be kept in the shielded gas area to avoid contaminating the filler wire.
Most of the other changes have to do with how the arc is started. With a high frequency start, the starting of an arc is not an issue. With manual or scratch start, the tungsten may contaminate the weld and loose its shape in the process. Most TIG welds are done with a side-to-side motion. If amperage is set properly and the weld puddle washes into the sides of the weld it should be fine.
Just like any other welding process there is not a single pattern or way to make a good weld. TIG welding works well in all positions on almost any metal. The only differences between a flat, horizontal, vertical and an overhead weld is how you mentally approach the task. Most of it comes down to a positive mind set and practicing. You want a smooth uniform bead that has washed into the joint properly.
Forehand or backhand ?
Forehand versus backhand welding shows little difference. Since TIG welding uses a filler metal added by hand, it is the arc which determines the weld penetration. As long as the puddle washes into the metal smoothly it makes no difference how you travel. In non-TIG welding processes the angle of the travel is unforgiving, but TIG welding is very forgiving for torch angle and travel direction as long as the gas coverage is good.
Freehand
The freehand technique for TIG welding is exactly that, freehand. It’s pretty simple, just start a puddle and start adding filler metal with the other hand. Keep repeating.
Walking the cup
Walking the cup gives much more control than free hand welding, with much better weld quality and appearance. A weld that was done by walking the cup is almost robot like with the bead pattern very uniform and consistent. This is because the cup of the TIG torch is always leaning on the weld joint and the arc length is kept the same.
Arc length is the key when it comes to TIG welding bead appearance. To walk the cup you need to place the TIG torch cup on the weld joint and set the tungsten so that it is just above the weld joint. Then simply walk the cup and add or hold your filler wire in the joint. The cup gets its forward travel speed by moving the TIG torch handle in a way that creates a forward travel motion.
There are many ways to walk the cup but the ultimately it keeps the welder’s hands steady by providing a something to lean on at all times with a consistent arc length.
Trouble shooting
When TIG welding there is some common problems and weld defects. Most of these problems are easy to solve when you know what to look for. Some of the common problems include:
- Weld Porosity
Causes:
- Arc length is too long. Shorten your arc length.
- Joint is not cleaned properly. Clean with grinder or wire brush.
- Gas flow rate is too low or too high. In the event of the gas flow rate being too high the turbulence caused by the high flow rate will pull in air into the mix.
- Wrong cup size is being used. Change cup to proper size.
- Check for a draft coming into the weld area. If this is the case put up a barrier to stop the draft.
- Filler rod is oily, dirty, or corroded. Try a new filler rod.
- Shielding gas is contaminated. Change the gas.
- Wrong gas is being used. In most cases pure Argon is the proper gas typewrong gas is being used. In most cases pure Argon is the proper gas type.
- Cup or is not tight enough. Check all TIG torch parts for tightness./li>
- Hose lines may not be tightened or have a leak. Check connections for tightness or use soapy water to find any leaks.
- Tungsten Deteriorating or Unstable Arc
Causes:
- Gas flow is too low. Raise gas flow rate.
- Arc length to long. Shorten arc length.
- Wrong gas being used. Change the gas.
- Tungsten is contaminated. Break and reshape the tungsten.
- Tungsten contacted the puddle. Clean tungsten and shorten stick-out.
- Tungsten electrode diameter is too big or small. Replace tungsten with proper size.
- Wrong polarity. Change polarity or voltage type.
- Amperage is too low. Raise amperage.
- Ground clamp is not contacting properly. Clean ground connection.
- Weld metal is not cleaned properly. Grind or wire brush weld joint.
- TIG torch connection is loose. Tighten TIG torch connection at power supply.