Defects & cures
5 essentials of welding technique
5 essentials of welding:
- arc length
- current
- travel speed
- electrode
- edge preparation
Welding problems
Common welding problems:
- Porosity:
- Cause:
- short arc, long arc
- insufficient puddling time
- unprepared base metal
- incorrect current
- moisture in electrode
- high sulfur and lead bearing steel
- Cure:
- check impurities in base metal
- allow sufficient puddling time for gases to escape
- use proper current
- use weaving motion to eliminate pinholes
- use proper electrode; dry if moist
- hold arc longer
- Poor penetration:
- Cause:
- speed too fast
- electrode too big
- current too low
- faulty preparation
- Cure:
- use sufficient current.
- Weld slowly enough to get good root penetration.
- Calculate electrode penetration properly.
- Select electrode according to welding groove size.
- Leave proper free space at bottom of weld.
- Excessive penetration:
- Cause:
- excess current/voltage
- damp electrodes
- Cure:
- check welding current
- check condition of electrode coating
- Warping:
- Cause:
- shrinkage of weld metal
- faulty clamping of parts
- faulty preparation
- overheating of joint
- Cure:
- peen joint edges before welding
- increase travel speed
- avoid excessive space between parts
- clamp properly
- use back-up to cool parts
- adopt a welding procedure
- use high speed, moderate penetration electrodes.
- Poor appearance:
- Cause:
- faulty connections
- overheated
- wrong electrode
- improper use of electrode
- wrong arc and current voltage
- Cure:
- check arc length, electrode angle and travel speed
- avoid overheating
- use a uniform weave
- avoid overly high current
- Undercutting:
- Cause:
- faulty electrode manipulation
- faulty electrode usage
- current/voltage too high
- Cure:
- use a uniform weave in butt welding
- avoid using an overly large electrode
- avoid excessive weaving
- use moderate current; weld slowly
- hold electrode at a safe distance from the vertical plane in making horizontal fillet weld.
- Poor fusion:
- Cause:
- wrong speed
- current improperly adjusted
- faulty preparation
- improper electrode size
- Cure:
- adjust electrode and vee sizes
- weave must be sufficient to melt sides of joint
- proper current will allow deposition and penetration
- keep weld metal from curling away from plate.
- Distortion:
- Cause:
- uneven heating
- improper sequence
- deposited metal shrinks
- Cure:
- tack or clamp parts properly
- form parts before welding
- dispose of rolling or forming strains before welding
- distribute welding to prevent uneven heating
- examine structure and develop a sequence.
- Cracked welds:
- Cause:
- wrong electrode
- weld and parts' sizes unbalanced
- faulty welds
- faulty preparation
- rigid joint
- Cure:
- desined structure and welding procedure eliminate rigid joints
- heat parts before welding
- avoid welds in string beads
- weld from the center toward the edges
- make sound welds with good root fusion
- adjust weld size to parts size
- allow joints a proper and uniform free space.
- Weld cracking:
- Cause:
- damp electrodes
- high carbon sulfur or silicon
- excess current
- unsuitable electrode
- incorrect welding procedure
- Cure:
- check steel specification
- examine weld formation
- check electrode selection and welding procedure
- if necessary, preheat
- Parent metal cracking:
- Cause:
- high carbon, high manganese, high sulfur
- Cure:
- check hardness of weld adjacent zone
- check steel specification
- preheat
- use low-hydrogen or nickel-chrome electrodes
- use low current
- Crater cracking:
- Cause:
- poor welding technique
- excess current
- steel analysis
- damp electrodes
- insufficient puddling at end of weld
- Cure:
- fill craters to same section as weld proper
- check current
- check steel specification
- Electrode nibbing or feathering:
- Cause:
- eccentric cratering
- magnetic interference with DC
- Cure:
- visual examination of coating
- weld with electrode in different positions in holder
- check on AC
- Spluttering:
- Cause:
- excess current/voltage
- electrode too big
- travel speed too slow
- Cure:
- check current
- check welding procedure and technique
- Difficult arc starting:
- Cause:
- poor earth connection
- loose cable terminals
- flux on striking end
- poor contact in holder
- Cure:
- Arc instability:
- Cause:
- open circuit voltage too low
- current to low
- arc too short
- faulty circuit connections
- Cure:
- check open circuit voltage against electrrode recommendations
- check current and electrical connections
- check technique