CauseCorrective action
Distortion
Shrinkage of deposited metal pulls welded parts together and changes their relative positions.Properly clamp or tack parts to resist shrinkage of cooling metal.
Separate or perform parts sufficiently to allow for shrinkage of welds.
Peen the deposited metal while still hot.
Non-uniform heating of parts during welding causes them to distort or buckle before welding is finished. Final welding of parts in distorted position prevents control of desired dimensions.Support parts of structure to be welded to prevent buckling in heated sections, due to weight of parts themselves.
Improper welding sequence.Study the structure and develop a definite sequence of welding.
Distribute the welding to prevent excessive local heating.
Welding stresses
Joints too rigid.Slight movement of parts during welding will reduce welding stress.
Develop welding procedure that permits all parts to be free to move as long as possible.
Incorrect welding procedure.Make weld in as few passes as practicable.
Use special intermittent or alternating welding sequence and step-back or skip procedure.
Properly clamp parts adjacent to the joint. Use back-up to cool parts rapidly.
Inherent in all welds especially in heavy parts.Peen each deposit of weld metal. Stress-relieve finished product.
Warping (Thin plates)
Shrinkage of deposited weld metal.Distribute heat input more evenly over full length of the seam.
Excessive local heat at the joint.Weld rapidly with a minimum input to prevent excessive local heating of the plates adjacent to the weld.
Incorrect preparation of joint.Do not have excessive space between parts to be welded.
Prepare thin plate edges equal to ave and welding speed at all times.the thickness of the plates. No filler rod is necessary for this type of joint. Make a U-shaped corrugation in the plates parallel to and about 13mm away from the seam. This will serve as an expansion joint to take up movement during and after the welding operation.
Improper welding procedure.Use special welding sequence and step-back or skip procedure.
Improper clamping of parts.Properly clamp parts adjacent to the joint. Use back-up to cool parts rapidly.
Poor appearance
Poor welding technique: improper flame adjustment or welding rod manipulation.Use the proper welding technique for the welding rod used.
Do not use excessive heat.
Use a uniform weave and welding speed at all times.
Inherent characteristic of welding rod used.Use a welding rod designed for the type of weld.
Improper joint preparation.Prepare all joints properly.
Cracked welds
Joint too rigid.Design the structure and develop a welding procedure to eliminate rigid joints.
Weld too small for size of parts joined.Do not use too smnall a weld between heavy plates.
Increase size of welds by adding more filler metal.
Improper welding procedure.Do not make welds in string beads. Make welds full-size in short sections 200mm to 250mm long.
Welding sequence should be such as to leave ends free to move as long as possible.
Preheating parts to be welded sometimes helps to reduce high contraction stresses caused by localised high temperatures.
Poor welds.make sure welds are sound and the fusion is good.
Improper preparation of oints.Prepare joints with a uniform and proper gap. IOn some cases a gap is esential. In other cases, a shrink or press fit may be required.
Undercut
Excessive weaving of the blowpipe, improper tip size, and insufficient welding rod added to molten puddle.Modify welding procedure to balance weave of bead and rate of welding rod depositon, using proper tip size.
Do not use too small a welding rod.
Improper manipulation of the welding rod.Avoid excessive and non-uniform weaving.
Poor welding technique: Improper welding rod deposition with non-uniform heating.Do not hold a weaving rod too low near the lower edge of the plate in the vertical plane when making a horizontal filletweld, as undercut on the vertical plate will result.
Poor penetration
Improper preparation of joint.Be sure to allow the proper gap at the bottom fo the weld.
Deposit a layer of weld metal on the back side of the joint where accessible, to ensure complete fusion the lower 'V'.
Use of too large a welding rod.Select proper-sized welding rod to obtain a balance in the heat requirements for melting welding rod, breaking down side-walls, and maintaining the puddle of molten metal at the desired size.
Use small-diameter welding rodsn in a narrow welding groove.
Welding tip too small - insufficient heat input.UUse sufficient heat input to obtain proper penetration for the plate thickness being welded.
Too fast a welding speed.Welding speed should be lsow enough to allow welding heat to penetrate to the bottom of the joint.
Porous weld
Inherent properties of the particular type of welding rod.Use welding rod of proper chemical analysis.
Improper welding procedure and flame adjustment.Avoid overheating of molten puddle of weUse the proper flame adjustment and flux (if necessary) to ensure sound welds.
Insufficient puddling time to allow entrapped gas, oxides and slag inclusions to escape to the surface.Use the multi-layer welding technique to avoid carrying too large a molten puddle of weld metal.
Puddling keeps the weld metal molten longer and often ensures sounder welds.
Poor base metal.Modify the normal welding procedure to weld poor base metals of a given type.
Brittle welds
Unsatisfactory welding trod producing air-hardening weld metal.Avoid welding rods producing air-hardening weld metal where ductility is desired. High-tensile low-alloy steel rods are air-hardening and require proper base metal preheating, post-heating or both, to avoid cracking due to brittleness.
Excessive heat input with over-sized welding tip, causing coarse-grained and burnt metal.Do not use excessive heat input, as this may cause coarse-grained structure and oxide inclusion in weld metal deposits.
High-carbon or alloy base metal which has not been taken into consideration.A single-pass weld may be more brittle than a multi-layered weld, because it has not been refined by successive layers of weld metal.
Welds may absorb alloy elements from the parent metal and become hard. Do not weld a steel unless the analysis and characteristics are known.
Improper flame adjustment and welding procedure.Adjust the flame so that molten metal does not boil, foam or spark.
Poor fusion
Improper size of welding rod.When welding in narrow vees, use a welding rod small enough to reach the bottom.
Improper size of tip and heat input.Use sufficient heat to melt welding rod and to break down side walls of plate edges.
Improper welding technique.Be sure the weave is wide enough to melt the sides of a joint thoroughly.
Improper preparation of joint.The deposited metal should completely fuse with the side walls of plate to form a consolidated joint of base and weld metal.
Brittle joints
Air-hardening base metal.In welding on medium carbon steel or certain ally steels, the fusion zone may be hard as the result of rapid cooling. Preheating at 150-260oC should be resorted to before welding.
Unsatisfactory welding rod.The use of austenitic welding rods will often be satisfactory on special steels, but the fusion zone will generally contain an alloy which is hard.
Corrosion
Type of welding rod.Select welding rods with the proper corrosion-resisting properties, which are not changed by the welding process.
Improper weld deposit for the corrosive fluid or atmosphere.Use the proper flux on both parent metal and welding rod to produce welds with the desired corrosion resistance.
Do not expect more from the weld than you do from the parent metal. On stainless steels, use welding rods that are equal to or better than the base metal.
For best corrosion resistance use a filler rod whose composition is the same as that of the base metal.
Metallurgical effect of welding.When welding 18/8 austenitic stainless steel, be sure the analysis of the steel and the welding procedure are correct, so that welding does not cause carbide precipitations. This condition can be corrected by annealing at 1040 - 1150oC.
Improper cleaning of weld.Certain materials such as aluminium require careful cleaning of all slag to prevent corrosion.

Back to metal & wood index